통계적 근거에 의한 표층 아스팔트 혼합물 변형강도의 배합강도 설정연구
라일호, 김진철, 도영수 et al. · 한국도로학회논문집 · 2009
This study was performed to establish the process mean which is statistically satisfying the critical limit of deformation strength (S D ), which is found to reflect rutting characteristics of asphalt mixture relatively well. The process means were determined using the critical S D values (3 ㎫ for local highway and 4 ㎫ for arterial highways), which were obtained from correlation analysis of APA and S D test data of actual highway projects, and coefficient of variation of 32 combinations of domestic mixtures. The process means of 3.2 ㎫ for local highway and 4.25 ㎫ for arterial highways were suggested when using 3 specimens (diameter of 100㎜). However, since these values are based on the loading speed of 30㎜/min, the higher values, 3.5 ㎫ for local highway and 4.5 ㎫ for arterial highways, were suggested, respectively, if the loading speed of 50㎜/min is applied using the old Marshall machine, which should give higher test values.