보문 : 상동광산 회중석광의 고압분해에 의한 텅스텐의 추출
정원배 · 1976
The effect of the condition of leaching solution (namely, Na₂CO₃concentration and Na₂CO₃equivalents to CaWO₄) on pressure leaching of table tailings from Sangdong mine (6.73% WO₃) with Na₂CO₃was investigated. The leaching was carried out in an autoclave, for 4 hours in a range of concentration from 25g/lto 250g/l, at 200℃, with 4 to 6 Na₂CO₃equivalents to CaWO₄. It has been found that increasing of Na₂CO₃concentration more than 100g/l, WO₃recovery was rapidly decresed. This phenomenon seems to be caused by the formation of complex compound, Na₂Ca(CO₃)₂·2H₂O, on the surface of ore particles as identified by X-ray diffraction.
Cited by 0 works.