以光電化學氧化法成長氮化鋁鎵/氮化鎵金屬-氧化物-半導體高速電子移動率場效電晶體閘極氧化層之製作與研究

黃立賢 · 2009

In this thesis, the photoelectrochemical (PEC) oxidation method was used to oxidize AlGaN directly forming insulators. According to the measured results of X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), and secondary ion mass spectrometry (SIMS), the as-grown films were indeed oxide layers which was consisted of Ga2O3 and Al2O3. There are few O-P bonds existed inner the oxide films because the electrolytic solution used in the PEC reaction is H3PO4. It is difficult to use the as-grown oxide films in the following device process because they dissolved easily in developer, alkaloid solutions and acid solutions. To overcome this problem, the as-grown oxide layer was annealed at 700oC in O2 ambient for 2 hours using furnace system. After the annealing process, the -Ga2O3 and -Al2O3 crystalline phases can be found in XRD patterns and the annealed oxide films were suitable for the following device process because they do not dissolve in developer, alkaloid solutions and acid solutions. The interface-state density, forward breakdown field and reverse breakdown field of the resulted AlGaN metal-oxide-semiconductor diodes with 45-nm-thick annealed gate insulators grown using the PEC oxidation method was 5.11011cm–2eV–1, 2.2MV/cm, and 6.6MV/cm, respectively. According to the results mentioned above, the oxide films grown using PEC oxidation method after proper annealing treatment have good insulations and interfaces with low interface-state density. The 45-nm-thick annealed oxide films were also used for gate insulation and surface passivation of AlGaN/GaN metal-oxide-semiconductor high-electron mobility field-effect transistors. The gate length and gate width was 3m and 300m, respectively. The drain-source current in saturation region (IDSS) at VGS0V was 200mA/mm and the maximum extrinsic transconductance was 50mS/mm obtained at VGS–2.09V and VDS10V. The gate voltage swing (GVS) was 2.4V. The Ion/Ioff ratio of the AlGaN/GaN MOS-HEMTs operated at VGS0V was 123.7. When the gate bias was 10V and 10V, the gate leakage current was only 50pA and 2pA, respectively. To realize the high-frequency performances of AlGaN/GaN metal-oxide-semiconductor high-electron mobility field-effect transistors, the transistors with 40-nm-thick annealed gate insulators and 1-m-long and 50-m-width two-finger gate pads were also fabricated. The IDSS at VGS0V was 580mA/mm and the maximum extrinsic transconductance of 76.72mS/mm was obtained at VGS–5.1V and VDS10V. The gate voltage swing (GVS) was 2.6V. The Ion/Ioff ratio of the AlGaN/GaN MOS-HEMTs operated at VGS0V was 134. The forward breakdown voltage and reverse breakdown voltage was 25V, and larger than –100V, respectively. Even operated at gate bias of 20V and 60V, the gate leakage current was only 960nA and 102nA, respectively. The unity current gain cutoff frequency (fT) and maximum frequency of oscillation (fmax) is 5.6GHz and 10.6GHz, respectively. To analyze the temperature dependence upon the performances of AlGaN/GaN metal-oxide-semiconductor high-electron mobility field-effect transistors, the direct-current (DC) electrical properties were measured at various temperatures. At 200oC, it can be seen that the IDSS at VGS=0V and the maximum extrinsic transconductance was only 408mA/mm and 46.83mS/mm, respectively. The decay of the IDSS and gm(max) was attributed to the decrease of the carrier mobility which was influenced by obvious phonons at high temperature. In addition, the gate leakage currents were also increased at high temperature because the electrons in the channel have enough energy for tunneling through the oxide layers. Finally, the low frequency noise in the linear region and saturation region of AlGaN/GaN metal-oxide-semiconductor high-electron mobility field-effect transistors were also measured and analyzed. The low frequency noise in the frequency ragne from 4Hz to 10kHz was fitted well by 1/f law as shown in the normalized noise power density spectra. In addition, the  values of 1/f fitting line at various gate-source biases were all close to unity. The Hooges coefficient (ch) was 4.63*10–4 and 3.16*10–4 in linear region (VDS=2V) when the gate bias was 8V and 1V, respectively. The Hooges coefficient (ch) is 8.79*10–4 and 9.32*10–4 in saturation region (VDS=10V) when the gate bias was -8V and 1V, respectively.

Cited by 0 works.

Authors