Синтез алюмо-скандиевых сплавов и лигатур в оксидно-фторидных расплавах
Суздальцев Андрей Викторович, Николаев Андрей Юрьевич, Зайков Юрий Павлович et al. · Transaction Kola Science Centre · 2015
Aluminium-scandium alloys (up to 0.5 wt % Sc) and master alloys (up to 2 wt % Sc) has been synthesized via chemical and electrochemical method in the KF-AlF3, NaF-AlF3 and KF-NaF-AlF3 melts with additions of Sc2O3 and Al2O3 in the temperature range 750–980°C. The electrolytic process was carried out in the lab-scale electrolyser with graphite anode and liquid aluminium cathode at 20 A current. The effect of cathodic current density (0–1 A/cm2), Sc2O3 content in the KF-NaF-AlF3 melt, aluminium stirring rate (0, 100 rpm) and the synthesis duration (30–180 min) on scandium content and distribution in the aluminium matrix, has been studied.
Cited by 0 works.