박리형 점착제에서 조성변화에 따른 물성에 관한 연구
서영옥, 설수덕 · Applied Chemistry · 1998
We were investigated performance of pressure-sensitive acrylic adhesive that blending of acrylic adhensive by batch reactor. and we examinated viscosity, temperature, heat treatment rate and peel adhesion. when the peel adhension is 160 g_f/25㎜ we know that optimum blending ratio is 1.3:1 as acrylic adhensive/solvent, that is shown hightest generality. when viscosity range of adhensive is 1000∼2000cps, peel adhension of removal type adhensive show ahout 160g_f/25㎜. For non-volatility after drying is 30%, viscosity show the optimum property so that we know a room temperature curing adhensive. Pot life is 30 sec. as a heat treatment rate at 50m/min, therefore minimum curing time is 30 sec. Not only weathering resistance keep up peel adhension 160∼180g_f/25㎜ after 1,000hrs, but also no residual remains.